Actual Yield
Strength, ksi (MPa)
Maximum
Thickness, in. (mm)
Minimum Average
Absorbed Energy,
ft-lbf (J)
Test Temperature,
°F (°C)
All1/2 (13)No recommendation provided
≤ 65 (≤ 450)2 (50)15 (20)10 (−12)
4 (100)20 (27)10 (−12)
65 < Fy ≤ 70 (450 < Fy ≤ 485)2 (50)20 (27)−10 (−23)
4 (100)25 (34)−10 (−23)
70 < Fy ≤ 100 (485 < Fy ≤ 690)4 (100)25 (34)−10 (−23)

2. PDF page 369

SpecificationGradeFy,
ksi (MPa)
Fu,
ksi (MPa)
ASTM A53/A53MB35 (240)60 (415)
ASTM A500/A500M
(square, rectangular, round)
B46 (315)58 (400)
C50 (345)62 (425)
ASTM A501/A501MA36 (250)58 (400)
B50 (345)70 (485)
ASTM A618/A618M
(round)
I and II50 (345)70 (485)
[t ≤ 3/4 in. (19 mm)] III50 (345)65 (450)
ASTM A847/A847M50 (345)70 (485)
CAN/CSA-G40.20/G40.21350W51 (350)65 (450)
ASTM A1085/A1085MA50 (345)65 (450)
ASTM A1065/A1065M5050 (345)60 (415)